Performance Test Results
Project |
Quality indicator |
Quality indicator |
Quality indicator |
Quality indicator |
Quality indicator |
Quality indicator |
Viscosity class |
15 |
22 |
32 |
46 |
68 |
100 |
Flash point (opening) /℃ is not less than |
125 |
175 |
175 |
180 |
180 |
190 |
Kinematic viscosity (40℃)/(mm2/s) |
13.5~16.5 |
19.8~24.2 |
28.8~35.2 |
41.4~50.6 |
61.2~74.8 |
90~110 |
When the kinematic viscosity is 1500mm2/s, the temperature /℃ is not higher than that |
-30 |
-24 |
-18 |
-12 |
-6 |
0 |
Viscosity index is not less than |
130 |
140 |
140 |
140 |
140 |
140 |
Pour point /℃ is not higher than |
-36 |
-36 |
-33 |
-33 |
-30 |
-21 |
Moisture (mass fraction) /% is not greater than |
vestige |
vestige |
vestige |
vestige |
vestige |
vestige |
Copper corrosion (100℃, 3h)/grade is not greater than |
1 |
1 |
1 |
1 |
1 |
1 |
Liquid phase rust (24h) |
1 |
1 |
1 |
1 |
1 |
1 |
Liquid phase corrosion test ( 24h ) |
rustless |
rustless |
rustless |
rustless |
rustless |
rustless |
Foaming properties (foaming tendency/foaming stability) (ml/ml)
|
150/0
75/0
150/0 |
150/0
75/0
150/0 |
150/0
75/0
150/0 |
150/0
75/0
150/0 |
150/0
75/0
150/0 |
150/0
75/0
150/0 |
Resistance to emulsification (time to 3ml) /min
|
30 30 |
30 30 |
30 30 |
30 30 |
30 30 |
30 30 |